Small-Scale Thinking

Nano-technology pretreatment improves powder coating quality and productivity.

By Jim Destefani, Editor


Vanadate Conversion Coatings: Alternative to Phosphate?
Fluorozirconium-based conversion coatings
available in today’s marketplace offer an alter-
native to traditional iron phosphate conversion coatings. The economic and environmental benefits of alternative conversion coat-
ings, such as vanadate, are intriguing, but each metal finishing operation has its own quality requirements and process capabilities. Potential users need to undertake a careful evaluation to determine if the new conversion coatings can offer the level of cor-
rosion resistance performance desired,
operate within existing or desired process equipment and deliver the expected ROI.

get info

...Visit Henkel Technologies' PF Online Showroom, call 248- 583-9300, or select the Product icon on the right.

Cleaning/Pretreatment Zone
powder coating zone

print this article

In the past couple of years, managers at the Flexcel plant in Post Falls, ID, have completely re-invented the finishing process for their products.

The company first replaced its liquid paint application process with powder coating, completing the transition near the end of 2004. The result, according to first-shift Manufacturing Manager Garrett Brown, was a substantial increase in product quality. “The switch from paint to powder boosted quality yield from approximately 93% to 98%,” he recalls.

The plant manufactures metal office furniture, panel systems and file storage products for its parent company Kimball International (Jasper, IN) as well as for other office furniture OEMs. The facility is divided into three main sections—metal fabrication, finishing and assembly. Work materials are mainly cold-rolled steel and aluminum extrusions.

employee performs a quality check
Process engineer David Mills watches while a flexcel employee performs a quality check on the company’s large pretreatment line. The line handles 2,000 to 2,200 parts carriers a day.

Post Falls operates in a make-to-order environment using lean manufacturing principles and techniques. The plant runs three finishing lines: a batch line for fast-turnaround, short run jobs; a mid-size line and a large main line with more than a mile of conveyor. Cycles on the three lines, from the time parts are hung on hooks until they are removed after cooling, are one, two, and three hours, respectively. Throughput on the main line is 2,000–2,200 carriers a day. The other lines process another 100–200 carriers daily working two shifts.

The nature of the plant’s business–building custom furniture a variety of customers–results in an average of about 65 color changes a day on the powder line, says Process Engineer David Mills. “With that many color changes, we don’t reclaim powder,” he explains. “Our transfer efficiency runs between 40 and 60%.”

Environmental Issues
You might think figuring out what to do with that waste powder would be a problem, but it isn’t, says Plant Environmental Manager Terry Hentges. “They use the powder to help power the waste-to-energy facility in Spokane (WA),” he explains. “It burns really well, and they’ll take all of it we give them.”

Hentges adds that doing away with liquid paint processes substantially reduced the plant’s environmental footprint by cutting volatile organic compound (VOC) emissions by approximately 200,000 lb/yr. The plant also switched from a water-based glue process to double-sided tape for panel assembly operations, resulting in less landfill waste from this process and a safer work environment for employees.

Those changes left the plant’s iron phosphate powder pretreatment process as Hentges’ biggest headache. “Only 650 ft of pipeline separate the plant from the nearest wastewater treatment plant,” he explains. “If we would have a discharge of, for example, hot water, it would impact their operations. And, most treatment plants aren’t set up to handle phosphates.” Even worse, he says, the state of Washington is considering a new threshold on phosphates that would essentially reduce allowable discharges to zero. (Post Falls is on the Spokane River near the Washington/Idaho border, about 20 miles east of Spokane, and the only wastewater treatment facility between Flexcel and the Columbia River 40 miles away is the one near the plant.)

end-on view of the booth
As this end-on view of the booth shows, Flexcel uses both automated and manual powder application. The plant changes colors an average of more than 60 times a day.

But environmental concerns weren’t the only reason managers began taking a hard look at the plant’s pretreatment process. Quality and energy cost issues also impacted their decision-making process.

“Our previous pretreatment system consisted of a cleaning stage with a mild surfactant, then the iron phosphate stage, then two rinse stages, then a rinse with deionized water,” Mills recalls. “With the new process, we use an alkaline cleaner, rinse, then the new nano-ceramic conversion coating, then a fresh water rinse. We don’t have to use DI to meet performance requirements.”

The new conversion coating is Bonderite NT-1, a reactive nano-ceramic process that is free of phosphate, regulated heavy metals and organic components. The nanometer-scale deposit produced by the process is more cost-effective than conventional iron phosphating, and provides corrosion resistance equal to or better than an iron phosphate/polymer seal, according to developer Henkel Corp. (Madison Heights, MI).

Henkel says the pretreatment is suitable for all conventional powder and wet paint coatings, can be applied by immersion or spraying and creates an inorganic, extremely high-density layer incorporating nano-particles. It results in a conversion layer on the order of nanometers thick, as opposed to phosphate, which is on the order of microns
thick.

The process coats steel, aluminum and zinc-coated substrates, and is said to deliver better corrosion protection and paint adhesion than iron phosphating. It runs at ambient temperature and eliminates a passivation step, further decreasing costs. Its low-sludge characteristics reduce waste disposal, cleaning and maintenance.

Making The Switch
According to Mills, the transition to the new pretreatment process required some modifications to the plant’s existing equipment. "We needed a stainless steel tank to hold the NT-1, which is acidic,” he says. “The main issue involved the tanks on our mid-size monorail line. They’re mild steel, so we had to line them. But our other tanks were stainless steel, so we didn’t have to do anything with them.” Some pump parts also required modification, he adds.

Post Falls managers proved out the new process on their mid-size finishing line before rolling it out on their large system. “The conversion was one of the smoothest I’ve seen,” Mills recalls. “We did a lot of testing, and then we did the conversion over a weekend.

“We also had to test parts to prove they met our salt spray, humidity chamber and other requirements,” he continues. “We had to get approvals from the city, from the state and from Kimball corporate environmental. So we basically proved out the new pretreatment on our smaller monorail system. It handles less than 10% of our volume, so it was a good test platform.”

Multiple Benefits
The pretreatment worked as advertised at Post Falls, providing operating and environmental benefits that resulted in a quick return on investment.

mid-size monorail line
Parts run through the plant’s mid-size monorail line, which was used as a platform to prototype the nano-technology pretreatment process before it was rolled out to other plant systems.

“Energy savings was a key,” Mills says. “The old process had cleaning and phosphate stages heated to about 140°F. Now, we’ve eliminated process heating. We’re saving close to $50,000 a year in gas costs.

“Our process is also more consistent and easier to control, and we were able to standardize our mid-size and large lines with one chemistry. Before, we had different chemical makeups on each of three systems,” he adds.

In terms of part quality, the switch virtually eliminated water spots and adhesion failures, according to Mills. He attributes the quality improvements to use of a more aggressive alkaline cleaner, which provides better surface quality than the mild surfactant used previously.

Environmentally, the process produces much less sludge than the previous pretreatment. “We still pump out our tanks once a year, but we don’t have to have a tanker truck to haul away the sludge as hazardous waste,” Brown explains. “Now all we have to do is neutralize the pH.”



Zones | Suppliers | Products | Articles | Forums | Events | Clinics | Subscribe | Advertise | Contact Us

Products Finishing Magazine. The Web Resource For Product Finishing Professionals
®2008 Gardner Publications, Inc